Hydrofluoric acid (HF) is very corrosive and can react with many metals, including cast iron, to generate hydrogen gas. Common stainless steel types, like 304 and 316, are not resistant to HF at any concentration or temperature. Higher grades of stainless steel may have some resistance, but they can still be attacked locally. 

Corrosion rates in Hydroflouric Acid (HF)

Corrosion rates in Hydroflouric Acid (HF)

AlloyNotesConcentration, %TemperatureTimeCorrosion RateRef
  CFmm/yrmils/yr
316 3 21 70 1.25 49.1 1
316 5 21 70 2.33 91.8 1
316 5 40 104 7.8 306 1
316 1 50 122 1.82 71.8 1
316 2 50 122 5.3 209 1
316 5 50 122 15.9 626 1
904L 3 21 70 0.125 4.9 1
904L 5 21 70 0.18 7.2 1
904L 5 40 104 0.73 28.8 1
904L 1 50 122 0.23 9.2 1
904L 2 50 122 0.71 28 1
904L 3 50 122 0.85 33.5 1
904L 4 50 122 1.36 53/5 1
904L 5 50 122 1.82 71.6 1
904L 1 70 158 0.99 39 1
904L 2 70 158 2.0 80.2 1
904L 3 70 158 3.31 130 1
AL-6XN 3 21 70 0.08 3.2 1
AL-6XN 5 21 70 0.20 8.0 1
AL-6XN 5 40 104 0.82 32.4 1
AL-6XN 1 50 122 0.10 4.1 1
AL-6XN 2 50 122 0.43 16.9 1
AL-6XN 3 50 122 0.98 38.4 1
AL-6XN 4 50 122 1.42 55.9 1
AL-6XN 5 50 122 2.0 78.7 1
AL-6XN 1 70 158 0.54 21.1 1
AL-6XN 2 70 158 1.98 78 1
AL-6XN 3 70 158 3.05 120 1
C-276 2 70 158 0.23 9 7
C-276 5 70 158 0.25 10 7
C-22 2 70 158 0.23 9 7
C-22 5 70 158 0.36 14 7
625 2 70 158 0.51 20 7
625 5 70 158 0.41 16 7
400 saturated with air 25 30 86 24hr 1 37 17
400 saturated with air 25 80 176 24hr 0.28 11 17
400 saturated with air 50 30 86 24hr 0.2 8 17
400 saturated with air 50 80 175 24hr 1 39 17
400 purged with nitrogen 25 30 86 48hr 0.005 0.2 17
400 purged with nitrogen 25 80 176 48hr 0.061 2.4 17
400 purged with nitrogen 50 30 86 48hr <0.003 <0.1 17
400 purged with nitrogen 50 80 176 48hr 0.01 0.5 17
Privacy Overview

This website uses cookies so that we can provide you with the best user experience possible. Cookie information is stored in your browser and performs functions such as recognising you when you return to our website and helping our team to understand which sections of the website you find most interesting and useful.